Material Number Material Number (single) Standard Range of Application Standard Status Country Successor
0.7043 (DIN 1693-1 : 1973-10) 0.7043 DIN 1693-1 : 1973-10 DIN 1693-1 : 1973-10 replaced by DIN EN 1563 : 2005-10 Replaced Germany EN-GJS-400-18-LT 1)
1) Remark: GGG-40.3, a cast iron material with nodular graphite with ensured notch impact energy at -20 °C and high toughness. Use for spring rockers, engine housings for rope hoists, water pump cases, bodies for machine tools, like stand, framework, housing, cross beams.

Chemical Composition

C [%] Mg [%] Mn [%] P [%] S [%] Si [%]
blur blur blur blur blur blur 1)2)
1) Source: blur
2) Remark: blur

Mechanical Properties

Semi-finished Product Condition Temperature [°C] Tensile Strength [MPa] Yield Strength [MPa] Yield Strength (0.2% offset) [MPa] Elongation A [%] Hardness HB | HBW
blur blur blur blur blur blur blur blur 1)2)
blur blur blur blur blur blur blur blur 1)2)
blur blur blur blur blur blur blur blur 3)4)
blur blur blur blur blur blur blur blur 3)4)
blur blur blur blur blur blur blur blur 3)4)
blur blur blur blur blur blur blur blur 3)4)
blur blur blur blur blur blur blur blur 3)4)
blur blur blur blur blur blur blur blur 3)4)
blur blur blur blur blur blur blur blur 3)4)
blur blur blur blur blur blur blur blur 3)5)
blur blur blur blur blur blur blur blur 3)5)
blur blur blur blur blur blur blur blur 3)5)
blur blur blur blur blur blur blur blur 3)5)
blur blur blur blur blur blur blur blur 3)5)
blur blur blur blur blur blur blur blur 3)5)
blur blur blur blur blur blur blur blur 3)5)
1) Source: blur
2) Remark: blur
3) Source: blur
4) Remark: blur
5) Remark: blur

Physical Properties

Temperature [°C] Poisson's Ratio Mean Coefficient of Thermal Expansion (reference 20°C) [10^-6*K^-1] Thermal Conductivity [W/(m*K)]
blur blur blur blur 1)
blur blur blur blur 1)
blur blur blur blur 1)
blur blur blur blur 1)
blur blur blur blur 1)
blur blur blur blur 2)
1) Source: blur
2) Source: blur

Toughness Data (Impact)

Semi-finished Product Condition Temperature [°C] Specimen Shape Notch Impact Energy [J]
blur blur blur blur blur 1)2)
blur blur blur blur blur 1)3)
blur blur blur blur blur 1)2)
blur blur blur blur blur 1)3)
1) Source: blur
2) Remark: blur
3) Remark: blur

Heat Treatment

Heat Treatment Step Temperature [°C] Holding Time [h] Medium
blur blur blur blur blur 1)2)
blur blur blur blur blur 1)3)
blur blur blur blur blur 1)4)
blur blur blur blur blur 1)5)
blur blur blur blur blur 1)6)
blur blur blur blur blur 1)7)
1) Source: blur
2) Remark: blur
3) Remark: blur
4) Remark: blur
5) Remark: blur
6) Remark: blur
7) Remark: blur

Cross Reference

Material Name Country Standard
Grade 370/17 Great Britain BS 2789-85
FCD 370 Japan JIS G 5502-89
0717-15 Sweden MNC 706E-89
EN-GJS-400-18-LT (EN-JS1025) Germany DIN EN 1563

Material Compliance

REACh RoHS
blur blur

FKM Guideline Fatigue Strength

Semi-finished Product Condition Nominal Size [mm] Tensile Strength [MPa] Yield Strength (0.2% offset) [MPa] Elongation A [%] Fatigue Limit under rev. Tension-Compression Stresses [MPa] Fatigue Strength under pulsating Tensile Stresses [MPa] Bending Fatigue Strength [MPa] Shear Fatigue Strength [MPa] Torsion Fatigue Strength [MPa]
blur blur blur blur blur blur blur blur blur blur blur 1)2)
1) Source: blur
2) Remark: blur

Linear-elastic

Temperature [°C] Young's modulus [GPa] Bulk modulus [GPa] Shear modulus [GPa] Poisson's ratio
blur blur blur blur blur
blur blur blur blur blur

Yield strength

Temperature [°C] 0.1% Proof strength [MPa] 0.2% Proof strength [MPa] Yield strength [MPa]
blur blur blur blur
blur blur blur blur
blur blur blur blur
blur blur blur blur
blur blur blur blur
blur blur blur blur
blur blur blur blur
blur blur blur blur

Coefficient thermal expansion

Related Temperature [°C] Temperature [°C] Coefficient thermal expansion [10^-6*K^-1]
blur blur blur
blur blur blur
blur blur blur
blur blur blur
blur blur blur

Tensile strength

Temperature [°C] Tensile strength [MPa]
blur blur

Thermal conductivity

Temperature [°C] Thermal conductivity [W/(m*K)]
blur blur
blur blur
blur blur
blur blur
blur blur

Classification

WIAM Material Treatment Semi-finished product Dimension [mm] Load type Failure criteria Rolling direction Maximum stress [MPa] Strain at maximum stress [%] Source description
blur blur blur blur blur blur blur blur blur blur

Designation

Designation Material number Source
blur blur blur
blur blur blur
blur blur blur
blur blur blur
blur blur blur
blur blur blur
blur blur blur
blur blur blur
blur blur blur
blur blur blur
blur blur blur
blur blur blur
blur blur blur
blur blur blur
blur blur blur

Yield strength

Temperature [°C] 0.1% Proof strength [MPa] 0.2% Proof strength [MPa] Yield strength [MPa]
blur blur blur blur

Tensile strength

Temperature [°C] Tensile strength [MPa]
blur blur

Classification

WIAM Material Treatment Semi-finished product Dimension [mm] Load type Failure criteria Rolling direction Maximum stress [MPa] Strain at maximum stress [%] Source description
blur blur blur blur blur blur blur blur blur blur

Tensile strength

Temperature [°C] Tensile strength [MPa]
blur blur

Classification

WIAM Material Treatment Semi-finished product Dimension [mm] Load type Failure criteria Rolling direction Maximum stress [MPa] Strain at maximum stress [%] Source description
blur blur blur blur blur blur blur blur blur blur

Yield strength

Temperature [°C] 0.1% Proof strength [MPa] 0.2% Proof strength [MPa] Yield strength [MPa]
blur blur blur blur
blur blur blur blur
blur blur blur blur
blur blur blur blur
blur blur blur blur
blur blur blur blur
blur blur blur blur

Classification

WIAM Material Treatment Semi-finished product Dimension [mm] Load type Failure criteria Rolling direction Maximum stress [MPa] Strain at maximum stress [%] Source description
blur blur blur blur blur blur blur blur blur blur

Yield strength

Temperature [°C] 0.1% Proof strength [MPa] 0.2% Proof strength [MPa] Yield strength [MPa]
blur blur blur blur

Tensile strength

Temperature [°C] Tensile strength [MPa]
blur blur

Classification

WIAM Material Treatment Semi-finished product Dimension [mm] Load type Failure criteria Rolling direction Maximum stress [MPa] Strain at maximum stress [%] Source description
blur blur blur blur blur blur blur blur blur blur